Image

laser= 457nm dpss 200mw
exposer= 40sec
formula= 1.3/13/100
angle= 56
meter reading=1.18
energy=50mj
humitity=49
coffee=hot :D

process
wash 1min
blot off excess water
iso 35% 10sec
iso 70% 10sec
iso 91% 10sec
2 min blast of hot air
1 min micro wave high
1 min micro wave high
seal hologram with "Zip Dry Paper Glue"
MichaelH

DCG Master

Post by MichaelH »

What did you do to the hologram between the two microwavings?
Danny Bee

DCG Master

Post by Danny Bee »

MichaelH wrote:What did you do to the hologram between the two microwavings?
some time if glass gets too hot it will crack ...so i do 1 min intervals and just open door for a few seconds
Dutchelm05

DCG Master

Post by Dutchelm05 »

Great piece Danny,

Can you discribe how this DCG master is optically set up?
I am guessing it is a transmission hologram set up.

Thanks,
Tony
Locked